In my experience, grinding of SiC is the standard method for backthinning.
However, due to the fragility of the material, it is necessary to attach the
material to some sort of carrier substrate prior to the back thinning process;
otherwise, the SiC wafer would easily break in response to any experienced
stress. Another necessary step would be to be able to remove this carrier at a
later point for singulation and packaging of the devices.

EVG has developed an automated method with which to perform this temporary (i.e.
reversible) bonding and debonding process.  Our system is capable of utilizing a
variety of bonding methods to achieve the desired results.  We have also
developed a debonding system to compliment the bonding system, allowing the
capability to remove the carrier and handle the fragile released substrates.

Best Regards,

Chad Brubaker

EV Group       invent * innovate * implement
Technology - Tel: (602) 437-9492, Fax: (602)437-9435 e-mail:
[email protected], www.EVGroup.com

This message and any attachments contain confidential or privileged information,
which is intended for the named addressee(s) only. If you have received it in
error, please notify the sender immediately and then delete this e-mail. Please
note that unauthorized review, copying, disclosing, distributing or otherwise
making use of the information is strictly prohibited.

 -----Original Message-----
From:   [email protected] [mailto:[email protected]]  On
Behalf Of Krasniansky Vladimir
Sent:   Tuesday, August 03, 2004 1:25 AM
To:     [email protected]
Subject:        [mems-talk] SiC backthinning

Hi all,
I'm looking for SiC backthinning method. Is anyone hear about grinding
of SiC? Is there other options except grinding or lapping?



Sincerely,

Vladimir Krasniansky,

Process Engineer,

Gal-El (MMIC);

100, Yitzhak Hanassi Blvd., P.O. Box 330 Ashdod 77102, ISRAEL.

Tel 972-8-857-2436/4

Fax 972-8-857-2658

[email protected]





 The information contained in this communication is proprietary to Israel
Aircraft Industries Ltd.
and/or third parties, may contain confidential or privileged information, and is
intended only for
the use of the intended addressee thereof. If you are not the intended
addressee, please be aware
that any use, disclosure, distribution and/or copying of this communication is
strictly prohibited.
If you receive this communication in error, please notify the sender immediately
and delete it from
your computer. Thank you.


This message is processed by the PrivaWall Email Security Server.


_______________________________________________
[email protected] mailing list: to unsubscribe or change your list
options, visit http://mail.mems-exchange.org/mailman/listinfo/mems-talk
Hosted by the MEMS Exchange, providers of MEMS processing services.
Visit us at http://www.memsnet.org/


reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
The Branford Group
Nano-Master, Inc.
University Wafer
Tanner EDA by Mentor Graphics