V, let me suggest longer and/or hotter hard bake on the hot plate not in the
oven. Gary

Gary Hillman
Service Support Specialties, Inc.
9 Mars Court
PO Box 365
Montville, NJ 07045
973-263-0640
973-263-8888.



-----Original Message-----
From:   [email protected] [SMTP:[email protected]]
Sent:   Thursday, August 12, 2004 10:58 AM
To:     [email protected]
Subject:        [mems-talk] 2um Al line etching using PR as a mask

Hello,

I have been trying to wet etch 300 nm thick Al layer using 2um wide PR
stripe. However I have problems width adhesion of resist to aluminum. PR
stripe seems to peal of when I'm etching.

I have been using following process.

1.    Spin HDMS on wafer (no I can't use vapor prime)
2.    Spin 1um thick AZ6612 on wafer
3.    Soft bake 2 min @ 110 C on hotplate
4.    Exposure
5.    Develop
6.    Hard bake 3 minutes in oven. 120 C.
7.    Etch with wet etchant

I have tried
HCl:H20 1:2 => very non uniform etching + Resist was removed
BOE => Resist was removed
HF:H2O2:H2O 1:1:20 => Resist was removed
H3PO4:HNO3:CH3COOH:H2O 4:1:4:1 => Resist was removed

Does anyone have good solutions. I know that I can grow SiN on Al and use
that as an etch mask or use dry etching but these steps make process more
complicated and I'm designing fast test process to test epi-wafers.

-Jukka Viheriala



_______________________________________________
[email protected] mailing list: to unsubscribe or change your list
options, visit http://mail.mems-exchange.org/mailman/listinfo/mems-talk
Hosted by the MEMS Exchange, providers of MEMS processing services.
Visit us at http://www.memsnet.org/

reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
MEMStaff Inc.
Mentor Graphics Corporation
Tanner EDA by Mentor Graphics
Process Variations in Microsystems Manufacturing