MEMSnet Home: MEMS-Talk: photoresist stripping with presence of Cu
photoresist stripping with presence of Cu
2004-09-03
Ebin Liao
2004-09-07
Borski, Justin
photoresist stripping with presence of Cu
Borski, Justin
2004-09-07
Hi Ebin,

some solvents and the direct presence of water can cause copper to corrode,
or "etch".  There are a couple things you could try, you might try rinsing
in isopropyl, or you might try searching for a vendor who sells "safe for
copper" solvent for resist strip.  There's a product called AZ S-46 Stripper
from Clariant which I believe is intended for use with copper films.

-Justin

Justin C. Borski
MEMS Program Manager
Advanced MicroSensors Inc.
[email protected]



-----Original Message-----
From: Ebin Liao [mailto:[email protected]]
Sent: Friday, September 03, 2004 4:35 AM
To: [email protected]
Subject: [mems-talk] photoresist stripping with presence of Cu


Hi, Dear MEMS fellows,

I have a question about photoresist stripping with
copper. When I strip the photoresist with PR-3000 with
the presense of Cu, I found some black spots on the Cu
pattern. At first I thought it's resist residue, but
later when I increase the stripping time, there are
even more black spots and also the copper pattern
dimension is somewhat reduced. Then I guess that the
copper may be attacked by the stripper.
Anyone can explain this phenomenon, its effect and
possible solutions? Thanks a lot.

Best regards,
Ebin

**********************AMS CONFIDENTIAL AND PROPRIETARY
INFORMATION*****************************
This e-mail communication and any attachments are confidential and intended only
for the use of the designated recipients named above.



reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
Harrick Plasma, Inc.
MEMS Technology Review
Addison Engineering
Tanner EDA by Mentor Graphics