unwanted tapering of SU-8 structures
2004-09-08
suscarl
2004-09-08
Patrick Poissant
2004-09-09
Jeff Babinski
unwanted tapering of SU-8 structures
Patrick Poissant
2004-09-08
Does your mask make a good contact with the samples? I had this problem when
my samples had edge bead. It sounds like also underexposed.

Patrick Poissant
___________________________________________________
   M.A.Sc. Student
   Dept. of Electrical Engineering
   Université de Sherbrooke
   Sherbrooke (Québec) J1K 2R1
   CANADA
   [email protected]
   Sherbrooke Microelectronics Research Group
   www.gel.usherb.ca/gms

   Anyone who has never made a mistake has never tried anything new - Albert
Einstein


----- Original Message -----
From: "suscarl" 
To: 
Sent: Wednesday, September 08, 2004 11:15 AM
Subject: [mems-talk] unwanted tapering of SU-8 structures


> Need advice from SU-8 experts:
> I have 30um width by 55um height SU-8 2035 lines. Somehow, after 35s
exposure time and post-bake of 95oC for 20min, the resulting structures are
tapered with bottom 60um width and top 40um width. Can anyone offer possible
solutions to troubleshoot the problem?
>
> Thanks!!
> _______________________________________________
> [email protected] mailing list: to unsubscribe or change your list
> options, visit http://mail.mems-exchange.org/mailman/listinfo/mems-talk
> Hosted by the MEMS Exchange, providers of MEMS processing services.
> Visit us at http://www.memsnet.org/
>
>


reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
Harrick Plasma, Inc.
MEMStaff Inc.
Nano-Master, Inc.
The Branford Group