MEMSnet Home: MEMS-Talk: nichrome deposition/adhesion for heater
nichrome deposition/adhesion for heater
2004-10-18
Amish Desai
nichrome deposition/adhesion for heater
Amish Desai
2004-10-18
Nichrome sputtering works well but has lot of
stress at thicker depositions.  Consequently, we
have experienced adhesion problems at 0.5um and greater.

Cheers,

Amish Desai
Tanner Research MEMS Fab



------------------------------

Message: 5
Date: Fri, 15 Oct 2004 09:58:59 -0700
From: "Kirt Williams" 
Subject: Re: [mems-talk] metallic microhotplate
To: "General MEMS discussion" 
Message-ID: <037d01c4b2d8$44d3ae60$6701a8c0@HPm495c2004>
Content-Type: text/plain;       charset="iso-8859-1"

Nichrome (80Ni 20Cr) will also work as a heater.
It has the benefit of good adhesion--no adhesion layer needs to be added.
A rough idea is of sheet resistance is 50 ohms/square at 650 A thickness.

I've also seen a paper in which pure chromium was used.

Tantalum, tantalum nitride, and TaAl alloy (used in some thermal inkjet
heads) are other options.

    --Kirt Williams

reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
Harrick Plasma, Inc.
Nano-Master, Inc.
MEMS Technology Review
Process Variations in Microsystems Manufacturing