Borski, Justin
Elevated temperature acetone bath for metallic liftoff process
Borski, Justin
2004-12-16
Hi Thomas,

You would be better served safety-wise by running an NMP-based process.  You
can safely run NMP solvent up to 70 degrees C without too much worry.  And
you should do this in an all-metal station.

- Justin

-----Original Message-----
From: Wilson, Thomas [mailto:[email protected]]
Sent: Wednesday, December 15, 2004 12:17 PM
To: General MEMS discussion
Subject: [mems-talk] Elevated temperature acetone bath for metallic
liftoff process


I've noticed that an ultrasonic acetone bath is too vigourous for my
particular metallic liftoff process with AZ5214E (1.4-micron thick) in
the case of a thin sputtered aluminum film (1000-A thick). Oftentimes,
the 10-micron wide patterned Al features also liftoff from the
substrate. I would like to know if anyone has experience with using
acetone at elevated temperature during liftoff (with the acetone beaker
immersed in a 37 degree C water bath)? Thank you.


Thomas E WILSON, Ph.D.
Professor of Physics and Physical Sciences
Marshall University
One John Marshall Drive
Huntington, WV  25755-2570
Tel: (304) 696-2752
FAX: (304) 696-3243

_______________________________________________
[email protected] mailing list: to unsubscribe or change your list
options, visit http://mail.mems-exchange.org/mailman/listinfo/mems-talk
Hosted by the MEMS Exchange, providers of MEMS processing services.
Visit us at http://www.memsnet.org/

**********************AMS CONFIDENTIAL AND PROPRIETARY
INFORMATION*****************************
This e-mail communication and any attachments are confidential and intended only
for the use of the designated recipients named above.



reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
The Branford Group
Process Variations in Microsystems Manufacturing
Mentor Graphics Corporation
Addison Engineering