MEMSnet Home: MEMS-Talk: Bulk Si-etch
Bulk Si-etch
2005-06-14
[email protected]
2005-06-15
Duan
Bulk Si-etch
Duan
2005-06-15
Hi Vinit,

54.7 is the angle between (111) plane to the wafer surface(100).  Due
to the atomic sturcture of silicon, the (111) plane is etched slowest
almost in every anisotropic etchant.  So you cann't get rid of 54.7
degrees.

However,  you can get vertical sidewalls if you align your opening to
(100) direction, not the wafer flat, then the (111) planes only occur
on the corner of the opening.  If you align your opening to other
directions, other angles will be possible, depending on the ER profile
of the etchant.

Another way is using (110) wafer, then you can get vertical sidewalls
which are (111) planes.  What kind of method you use, and what kind of
mask you should design will be related to your objective.

All these information can be in the literatures or the book
"fundamentals of MICROFABRICATION".

Good luck.

Duan

On 6/14/05, [email protected]  wrote:

> Is there any Si-etch method which etches anisotropically at angles lesser
> than 54 degrees ? I've looked around but the KOH-etch giving the steep
> 54.7 degree inclines is all that I've found.  I am looking to etch ~200
> microns deep.
reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
Process Variations in Microsystems Manufacturing
Mentor Graphics Corporation
Addison Engineering
Tanner EDA by Mentor Graphics