MEMSnet Home: MEMS-Talk: piezoresistance of polysilicon
piezoresistance of polysilicon
2005-07-16
yanli Wang
2005-07-17
Nikhil Mehta
2005-07-17
Behraad Bahreyni
piezoresistance of polysilicon
Behraad Bahreyni
2005-07-17
I have measured the piezoresistive coefficient of the poly1 layer in
MUMPS process to be about -11.5x10^-11 Pa. Check these papers for
information on piezoresistive coefficient of polysilicon in more general
cases:

V. A. Gridchin, V. M. Lubimsky, and M. P. Sarina, “Piezoresistive
properties of polysilicon films,” Sensors and Actuators A: Physical,
vol. 49, no. 1-2, pp. 67–72, June 1995.

  P. J. French, “Polysilicon: a versatile material for microsystems,”
Sensors and Actuators A: Physical, vol. 99, no. 1-2, pp. 3–12, April 2002.

  L. Latorre, Y. Bertrand, and P. Nouet, “On the use of test structures
for the electro-mechanical characterization of a CMOS compatible MEMS
technology,” in Proceedings of the IEEE International Conference on
Microelectronic Test Structures, vol. 1, March 1998, pp. 177–182.

Hope it helps.

Good luck,
Behraad
reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
MEMStaff Inc.
Process Variations in Microsystems Manufacturing
MEMS Technology Review
Nano-Master, Inc.