Erkin,

The problem here is that, especially with spin coating, the topography of the
posts will cause eddies to occur in the resist film leading to non-planarity.

There are a couple of approaches to look into:

1) Try aiming for a thicker layer.  However, this can be difficult, since with
spin coating, the resist film will tend to need to be much thicker than the
topography (probably >5 µm).

2) Spray coating: if you have this capability available to you, you would be
able to place down a 2-3µm layer of material that should maintain a good degree
of planarization during the soft bake.  We've had some pretty good results with
planarization of some pretty extreme topography.

I know I've listed this link before, but to keep it easy, take a look at the
following link to Micro Magazine:

http://www.micromagazine.com/archive/04/03/brubaker.html

Specifically, you'll want to look at figure 8b.

Best Regards,
Chad Brubaker
-----Original Message-----
From: erkin seker
Subject: [mems-talk] Surface Planarization

I have 1-um-thick, 100um-by-100um square SU8 posts, and I want to fill
around them with a sacrificial layer preferably photoresist.  When I spin
coat the photoresist (approximately 1-um-thick), and develop away the resist
over the posts, raised lips appear at the edges of the posts.  I tried
oxygen plasma to planarize the surface to some degree while depositing
multiple photoresist layers to reduce the lip formation, but it doesn't work
too well.
reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
Addison Engineering
MEMStaff Inc.
Process Variations in Microsystems Manufacturing
Tanner EDA by Mentor Graphics