sokwon Paik
Did anybody try to use MF319 for AZ1500 series developer?
2006-02-28
Bin Liu
2006-02-28
Brubaker Chad
2006-03-08
Jesse D Fowler
Anyone ever done bonding for 3" quartz wafer?
Jesse D Fowler
2006-03-08
Finally dug up the paper:

Jia, Z.; Fang, Q.; Fang, Z. Bonding of Glass Microfluidic Chips at Room
Temperatures, Anal. Chem. 2004, 76, 5597-5602.

This is about bonding glass, by pre-treating it in H2SO4 for 8-12 hours. I
don't know if this will give you any success with quartz. The paper has a
short review of bonding methods at the beginning that you may find
helpful.

Hope this helps,
Jesse Fowler

"Brubaker Chad" 
Sent by: [email protected]
02/28/2006 08:28 AM
Please respond to
General MEMS discussion 


To
"Chih-Chieh Cheng" , "General MEMS discussion"

cc
Brubaker Chad 
Subject
RE: [mems-talk] Anyone ever done bonding for 3" quartz wafer?


Chih-Chieh,

When trying to bond quartz, your options are pretty limited unless you
are using an intermediate layer.  Without such a layer, your only choice
is direct bonding.

To accomplish this, you would first need to do a reverse RCA clean as
follows:

RCA2 (SC-2): HCl (37%): H2O2 (30%):H2O in a volume ratio of 1:1:6 at 70C
for 5 minutes; DI water rinse

RCA1 (SC-1)              NH4OH (29%):H2O2 (30%):H2O in a volume ratio of
1:1:5 at
70C for 5 minutes; DI water rinse

I've actually done these steps a few times myself in the ASU CSSER clean
room; the chemicals should all be available.

Once the clean is done, you would place them into the EVG501 using
separation flags, cycle the chamber to achieve the desired atmosphere
(nitrogen, vacuum, etc.), apply contact at a single point using the
wafer bow function, and then pull the flags out one at a time. This
"pre-bond" would be applied at room temperature.

The key thing here is the smoothness and flatness of your wafers - the
process works best if the surface roughness is very low (<0.5 nm RMS),
but some bonding can still occur up to 2 nm RMS.

Once the pre-bond is done, the wafers would need to be placed in a
furnace at ~1000C for annealing.

If 1000C is not feasible, another option is via plasma activation prior
to the prebond (via an EVG810, for example), which will reduce the
anneal temperature to below 300C.

Best Regards,
Chad Brubaker

-----Original Message-----
From: [email protected]
[mailto:[email protected]] On Behalf Of Chih-Chieh Cheng
Sent: Monday, February 27, 2006 2:53 AM
To: [email protected]
Subject: [mems-talk] Anyone ever done bonding for 3" quartz wafer?

Hi, everyone

As title, we are trying to bond two 3" quartz wafer using EVG 501. Do
you
have any comments on it?
reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
Harrick Plasma, Inc.
The Branford Group
Process Variations in Microsystems Manufacturing
Mentor Graphics Corporation