A MEMS Clearinghouse® and information portal
for the MEMS and Nanotechnology community
RegisterSign-In
MEMSnet Home About Us What is MEMS? Beginner's Guide Discussion Groups Advertise Here
News
MEMSnet Home: MEMS-Talk: Re: AW: [mems-talk] polyimide
polyimide
2007-03-20
sheeja mathew
2007-03-21
Jason Milne
2007-03-21
Daniela Kögler
2007-03-22
Jason Milne
Re: AW: [mems-talk] polyimide
2007-03-22
sheeja mathew
Re: AW: [mems-talk] polyimide
sheeja mathew
2007-03-22
Hi,
       I don't know at which speed you have spun the polyimide and ppr.I think
the curing time was not sufficient in ur process.Precure the polyimide at 120
degrees for 30minutes.  Then it will not dissolve in organic solvents like
acetone.
  All the best.

  with regards ,
  D.sheela

Daniela Kögler  wrote:
  Hi,
I also work with the polyimid PI-2574.
I cured the polyimid at 110 degrees 3 minutes and it got etched and
transferred the pattern of a second photoresist layer. Unfortunately the
polyimid lost the adhesion to the si-wafer by the removal of the
photoresist.

I tried to cure the polyimid at 160 degrees; unfortunately it did not get
etched with the photoresist.

Is there a chance to etch the polyimid with photoresist developer AND remove
the photoresist afterwards?
reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
MEMS Technology Review
Process Variations in Microsystems Manufacturing
MEMStaff Inc.
Mentor Graphics Corporation