MEMSnet Home: MEMS-Talk: AZ5214E in image reversal mode
AZ5214E in image reversal mode
2007-05-16
Yue Mun Pun, Jeffrey
2007-05-16
Bill Moffat
2007-05-18
Zhang Xiao Qiang
2007-05-16
Chris Park
2007-05-16
Yue Mun Pun, Jeffrey
AZ5214E in image reversal mode
Yue Mun Pun, Jeffrey
2007-05-16
Hi,
I have tried to use AZ5214E in image reversal mode to pattern some alignment
marks by lift-off process.  I have compared the image reversal mode versus the
positive imaging mode and found that the lift-off process using image reversal
is much more difficult than the positive image mode.

Can anyone advise me on this matter?

Here is my image reversal process:
1.  Coat SiO2 wafer with AZ5214E spun at 2500rpm.  This gave me a resist of
thickness 1.4-1.6um.
2.  Soft bake at 95'C for 120s on hot plate.
3.  Expose at 405nm near UV light with intensity of about 7.5mW/cm2 for 5.4s to
obtain average energy of 40mJ/cm2.
4.  Reversal bake on hot plate at 115'C for 120s.
5.  Flood expose at 405nm with intensity of 7.5mW/cm2 for 160s to obtain average
energy of 1200mJ/cm2.
6.  Develop in AZ400K developer diluted in DI water to a ratio of 1:4 for
45-60s.
7.  Thermal evaporation of 30nm Chromium.
8.  Lift off via both Acetone and PGMEA (SU-8 developer).

The wafer with the positive image was run as above except without the reversal
bake aqnd flood exposure.

Lift-off using the image reveral mode is very difficult even after overnight
soak in PGMEA.

Jeffrey
reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
Nano-Master, Inc.
University Wafer
Process Variations in Microsystems Manufacturing
MEMS Technology Review