MEMSnet Home: MEMS-Talk: KOH and TMAH etch masks other than SiN for long Si etch
KOH and TMAH etch masks other than SiN for long Si etch
2009-04-21
l j
2009-04-21
Xiaoguang Liu
2009-04-21
Brian Stahl
2009-04-22
Yongliang Yang
KOH and TMAH etch masks other than SiN for long Si etch
2009-04-25
Chris P. Park
2009-04-22
Shao Guocheng
2009-04-22
Prem Pal
KOH and TMAH etch masks other than SiN for long Si etch
Prem Pal
2009-04-22
Dear KC

SiO2 exhibits excellent masking property in TMAH solution. I use thermally grown
oxide layers of about 0.9~1um thickness in 25 wt% TMAH at 80 C for more 10 hours
in order to etch {100}Si.

I think, in your case, oxide layer is very thin (500 A as you mentioned) and
porous. I suggest you to deposit thick oxide layer and do the etching in 5-10
wt% TMAH if etched surface roughness is not the issue, as the low concentration
provides high etch rate but rough etched surface morphology. If you have the
thermal annealing facility, anneal you oxide deposited wafers at 1000 C for
about one hour.

Cr-Au metal layer can use as mask in both KOH and TMAH. I think in your case
adhesion of deposited layer is not good. So before using the Cr-Au as mask,
check the adhesion of metal layer.  It can simply be done by scotch tape test
method.

Best regards
Prem

reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
MEMS Technology Review
Tanner EDA by Mentor Graphics
Process Variations in Microsystems Manufacturing
Harrick Plasma, Inc.