A MEMS Clearinghouse® and information portal
for the MEMS and Nanotechnology community
RegisterSign-In
MEMSnet Home About Us What is MEMS? Beginner's Guide Discussion Groups Advertise Here
News
MEMSnet Home: MEMS-Talk: photoresist peeled off during Ni e-beam deposition
photoresist peeled off during Ni e-beam deposition
2010-02-26
Wei Tang
2010-02-26
A.ALLOUCH
2010-02-28
basar bolukbas
2010-02-26
Wei Tang
2010-02-26
Johnson, Stafford
2010-03-01
A.ALLOUCH
2010-02-28
Wei Tang
2010-03-02
Wei Tang
photoresist peeled off during Ni e-beam deposition
basar bolukbas
2010-02-28
Dear Wei,

Did you try this deposition with a higher rate?

For example you can try 5A/sec.

I guess this will give you a better result. Otherwise i recommend increase your
deposition rate to 10A/sec.

Best Regards.

---

> Date: Thu, 25 Feb 2010 16:28:08 -0800
> From: [email protected]
> To: [email protected]
> Subject: [mems-talk] photoresist peeled off during Ni e-beam deposition
>
> Hi, all
>
> I have experienced a problem of photoresist peel off during the Nickel
> e-beam deposition (by CHA machine) process for lift-off purpose. The
> picture is shown:
>
> http://picasaweb.google.com/tangweipku/PRPeeledOffDuringEBeamDepositionOfNi#54
41568465466565330
>
> I am guessing the problem comes from the residual stress in the as
> deposited Ni film. The deposition rate is 3A/s and final thickness is
> 150nm. The PR is 1.4um AZ5214E and the pattern is made by
> image-reversal process. The SiO2 wafer have been primed in HMDS for
> 10min before spin coating. I have tried several method below but NONE
> of them solve the problem:
>
> (1) hard bake at 130C for 5min after development (the undercut has
> been compromised a lot during the hard bake process)
>
> (2) UV bake for 35min
>
> I am wondering is there any way to overcome this problem by:
> (1) adjust the deposition parameter to produce less stress
> (2) treat the photoresist to increase the adhesion with the substrate
> (I have already primed the wafer with HMDS before coating)
>
> Any comments or suggestions are appreciated.
>
> Thanks,
>
> Wei
reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
Addison Engineering
MEMS Technology Review
Nano-Master, Inc.
MEMStaff Inc.