MEMSnet Home: MEMS-Talk: PMMA cracking during e beam evaporation
PMMA cracking during e beam evaporation
2010-06-02
landobasa
2010-06-02
Barrios, Pedro
2010-06-02
sangeeth kallatt
2010-06-02
Mike Whitson
2010-06-02
Mike Whitson
2010-06-02
Christoph Stark
2010-06-02
[email protected]
2010-06-02
landobasa
2010-06-02
landobasa
2010-06-02
landobasa
2010-06-02
[email protected]
2010-06-03
Andrew Irvine
2010-06-03
Andrew Irvine
2010-06-03
Mike Whitson
PMMA cracking during e beam evaporation
landobasa
2010-06-02
Hi Sangeeth,

Unfortunately, I do not have thermal evaporator with me. I do not think we can
do it with sputtering, since it is conformal deposition.

Regards,

Lando

-------------------------

Hi Lando,

I am just wondering how can you do it with e beam evaporation. electron beam
beam can still react with PMMA and it can harden the polymer(PMMA acts as
negative tone resist under high dose)

It works well for me both RF sputtering and Thermal evaporation.

thanks,
sangeeth
reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
University Wafer
Mentor Graphics Corporation
MEMS Technology Review
Process Variations in Microsystems Manufacturing