Ryan D. Pooran
2002-03-04
Ted Harder
2002-03-04
Klauder, Jr., Philip R.
2002-03-04
[email protected]
Smooth KOH etching
[email protected]
2002-03-04
Ryan-
There are several papers on this subject.

In general, a KOH etched surface improves in roughness as you increase the
concentration. Of course, this increases the etch rate of your mask as well.
Increasing the concentration also diminishes diffusion effects( When etching
deep cavities in low concentration etchants, the center of the cavity will etch
at a different rate than the edges). Using greater than 30% by wt. KOH with
water should give you a smooth surface.

Intentional or unintentional additives can affect the surface quality. The
additional of various alcohols will change the etch properties. In addition,
contaminates such as iron in the solution can affect the surface of the etch.




"Ryan D. Pooran"  on 03/02/2002 08:28:22 PM

Please respond to [email protected]


To:   [email protected]
cc:    (bcc: Dan W Chilcott/DELCO)

Subject:  [mems-talk] Smooth KOH etching



Good day all,
  Recently I did a KOH etching of Si to make a thin diaphragm to be used
as a pressure sensor. The diaphragm that was etched was very rough on
the backside. Does anyone know how I can etch Si so it gives an almost
perfect smooth surface?

Thank you.
Ryan

Ryan D. Pooran
Graduate Student
Microelectronics- Photonics Graduate Program
University of Arkansas
248 Physics Building
Fayetteville, AR
72701
Ph: 501-575-5596(O)
Ph: 501-575-4150(L)
Email: [email protected]
_______________________________________________
[email protected] mailing list: to unsubscribe or change your list
options, visit http://mail.mems-exchange.org/mailman/listinfo/mems-talk
Hosted by the MEMS Exchange, providers of MEMS processing services.
Visit us at http://www.mems-exchange.org/




Received: from plmlir4.mail.eds.com ([205.191.22.44]) by ustryg98.delphiauto.net
(Lotus SMTP MTA v4.6.7  (934.1 12-30-1999)) with SMTP id 05256B72.0052BE01; Mon,
4 Mar 2002 10:03:46 -0500
Received: from plmler3.mail.eds.com (plmler3.mail.eds.com [199.228.142.73])
     by plmlir4.mail.eds.com (8.11.6/8.11.3) with ESMTP id g24F4LK06261
     for ; Mon, 4 Mar 2002 09:04:21 -0600 (CST)
Received: from kronos.mems-exchange.org (kronos.mems-exchange.org [132.151.8.1])

     by plmler3.mail.eds.com (8.11.6/8.11.3) with ESMTP id g24Ew6P31170
     for ; Mon, 4 Mar 2002 08:58:06 -0600
Received: from localhost ([127.0.0.1] helo=kronos.mems-exchange.org)
     by kronos.mems-exchange.org with esmtp (Exim 3.12 #1)
     id 16htud-0006H8-00; Mon, 04 Mar 2002 09:58:03 -0500
Received: from mail.uark.edu ([130.184.5.107]) by
  kronos.mems-exchange.org with esmtp (Exim 3.12 #1) id 16hKnp-0006oQ-00
  for [email protected]; Sat, 02 Mar 2002 20:28:41 -0500
Received: from delta ([130.184.14.127]) by mail.uark.edu (Netscape
  Messaging Server 4.15) with ESMTP id GSDIRQ01.W78 for
  ; Sat, 2 Mar 2002 19:28:38 -0600
From: "Ryan D. Pooran" 
To: 
Message-ID: <000001c1c252$b8d63f40$7f0eb882@delta>
MIME-Version: 1.0
Content-Type: text/plain; charset="us-ascii"
Content-Transfer-Encoding: 7bit
X-Mailer: Microsoft Outlook, Build 10.0.2627
Subject: [mems-talk] Smooth KOH etching
Sender: [email protected]
Errors-To: [email protected]
X-BeenThere: [email protected]
X-Mailman-Version: 2.0.8
Precedence: bulk
Reply-To: [email protected]
List-Unsubscribe: ,
     
List-Id: General MEMS discussion 
List-Post: 
List-Help: 
List-Subscribe: ,
     
List-Archive: 
Date: Sat, 2 Mar 2002 19:28:22 -0600


|--------------------------------------->
|USTRYG98/us/delphiauto                 |
|USTRYH99/us/delphiauto                 |
|USKOKH99/us/delphiauto                 |
|USKOKHM1/DELCO                         |
|USKOKM08/DELCO                         |
|--------------------------------------->
  >---------------------------------------|
  |03/04/2002 10:03:51 AM - 03/04/2002    |
  |10:03:51 AM                            |
  |03/04/2002 10:03:51 AM - 03/04/2002    |
  |10:04:00 AM                            |
  |03/04/2002 10:04:02 AM - 03/04/2002    |
  |10:04:06 AM                            |
  |03/04/2002 10:04:02 AM - 03/04/2002    |
  |10:04:04 AM                            |
  |03/04/2002 10:04:05 AM - 03/04/2002    |
  |10:04:06 AM                            |
  >---------------------------------------|

reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
Mentor Graphics Corporation
Tanner EDA by Mentor Graphics
Addison Engineering
Process Variations in Microsystems Manufacturing