MEMSnet Home: MEMS-Talk: Anodic Bonding - Glass Pits
Anodic Bonding - Glass Pits
2002-07-31
Brett Swope
2002-07-31
jun
Anodic Bonding - Glass Pits
jun
2002-07-31
Hi,  you need to use graphite electrode to avoid the pits.
we use both (steel and graphite electrodes) in U of Michigan, and the
results are consistent.

jun
----- Original Message -----
From: "Brett Swope" 
To: 
Sent: Wednesday, July 31, 2002 9:47 AM
Subject: [mems-talk] Anodic Bonding - Glass Pits


> I am attempting to set up an anodic bonding tool that will be able to
> uniformly bond 3" wafers.  At this point I am able to bond Corning 7070
> Borosilicate glass to Si wafers but after the wafers have cooled there
appears
> to be minor defects in the glass surface in the form of 'pits'.  Each pit
is
> less than 50 um in diameter and hundreds are spread randomly throughout
the
> glass.  My setup is as follows:
>
> Temp: 400 C
> Voltage: 500-1200 V
> Time: 1-5 mins
> Electrodes: 304 Stainless Steel (lapped and polished on glass contact
> surface)
>
> Has anyone ever heard of this?  I have looked through some literature but
> haven't found anything like this.
>
> Any help is appreciated!
> Brett Swope
> _______________________________________________
> [email protected] mailing list: to unsubscribe or change your list
> options, visit http://mail.mems-exchange.org/mailman/listinfo/mems-talk
> Hosted by the MEMS Exchange, providers of MEMS processing services.
> Visit us at http://www.memsnet.org/

reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
Nano-Master, Inc.
University Wafer
Harrick Plasma, Inc.
Tanner EDA by Mentor Graphics