Hi Dlee

You will not get very far using CF4 or SF6 to etch either Au or Cr.  Au and
Cr can be dry etched using a mainly physical process, using RIE with Ar gas.
You can add Cl2 to increase the rate if you have a load-locked system or a
glove-box.  In either case, the metal is likely to etch more slowly than the
PMMA.  PMMA is not very good at resisting plasma, especially if it gets hot.
Ideally, you want to clamp and cool the wafer, but not many systems offer
this.  Expect a rate of around 20nm/min or less (depending on process
conditions and loading).

Martin Walker B.Sc.(Tech.) M.Sc.
Oxford Instruments Plasma Technology
North End, Yatton, Bristol, BS49 4AP UK
T.+44 (0)1934 837031  F.+44 (0)1934 837001
E. 
W. 


 ###  OXFORD INSTRUMENTS   http://www.oxford-instruments.com/  ###

Unless stated above to be non-confidential, this E-mail and any
attachments are private and confidential and are for the addressee
only and may not be used, copied or disclosed save to the addressee.
If you have received this E-mail in error please notify us upon receipt
and delete it from your records. Internet communications are not secure
and Oxford Instruments is not responsible for their abuse by third
parties nor for any alteration or corruption in transmission.



reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
Tanner EDA by Mentor Graphics
MEMStaff Inc.
Addison Engineering
University Wafer