A MEMS Clearinghouse® and information portal
for the MEMS and Nanotechnology community
RegisterSign-In
MEMSnet Home About Us What is MEMS? Beginner's Guide Discussion Groups Advertise Here
News
MEMSnet Home: MEMS-Talk: Aluminum etched by developer
Aluminum etched by developer
2003-08-08
LSWANG
2003-08-09
alfred renaldo
2003-08-11
Jim Beall
2003-08-08
Michael D Martin
2003-08-10
Pavel Neuzil
2003-08-10
[email protected]
2003-08-11
Jobert van Eisden
Aluminum etched by developer
[email protected]
2003-08-10
Hi Lisen,

I had the same problem some time ago. Luckily for me the Al
layer was on the backside and the pattern I was developing
was on the front side.

So I protected the  backside of my wafer (Al pattern) with a
blanket coat of AZ 1512 (thinner than AZp4620) and then did
the lithography and development on the front side with
AZp4620 and AZ400k developer. After this to remove the
protective layer on the Al side I did an O2 clean in the RIE
for 5 mins. This easily removed the resist on the Al side
leaving the pattern on the frontside intact.

If you have both patterns on the same side then you might
want to take into account the Al etchrate while designing
your mask.However if you have only 1 pattern in Al (and no
other lithography steps) then the unexposed resist should
protect the Al in the places you want it pretty well.

Hope this helps

Goodluck
Anupama


> Hi,there,
> Anyone has experience with patterning Al. I got
> problem when developing the photoresist, the Al layer
> is etched by the developer. I tried SHipley and AZ
> resists, but both have the same problem. THanks
> Lisen
>
> __________________________________
> Do you Yahoo!?
> Yahoo! SiteBuilder - Free, easy-to-use web site design
> software http://sitebuilder.yahoo.com
>
> _______________________________________________
> [email protected] mailing list: to unsubscribe or
> change your list options, visit
> http://mail.mems-exchange.org/mailman/listinfo/mems-talk
> Hosted by the MEMS Exchange, providers of MEMS processing
> services. Visit us at http://www.memsnet.org/

reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
MEMStaff Inc.
Addison Engineering
Harrick Plasma, Inc.
Process Variations in Microsystems Manufacturing