A MEMS Clearinghouse® and information portal
for the MEMS and Nanotechnology community
RegisterSign-In
MEMSnet Home About Us What is MEMS? Beginner's Guide Discussion Groups Advertise Here
News
MEMSnet Home: MEMS-Talk: CORRECTION: fabricating optics with reflowed photoresist in plasmaetcher, problem with surface roughness
fabricating optics with reflowed photoresist in plasma etcher, problem with surface roughness
2004-04-04
Patrick Lu
CORRECTION: fabricating optics with reflowed photoresist in plasmaetcher, problem with surface roughness
2004-04-05
Patrick Lu
CORRECTION: fabricating optics with reflowed photoresist in plasmaetcher, problem with surface roughness
Patrick Lu
2004-04-05
Sorry, I meant CF4 not CH4. :)

Patrick Lu
Stanford University
Department of Electrical Engineering
http://www.stanford.edu/~patlu

-----Original Message-----
From: [email protected]
[mailto:[email protected]] On Behalf Of
Patrick Lu
Sent: Sunday, April 04, 2004 12:39 AM
To: [email protected]
Subject: [mems-talk] fabricating optics with reflowed photoresist in
plasmaetcher, problem with surface roughness

Hi,



I have quartz wafers covered with reflowed photoresist. I am etching these
with a mixed CH4 and O2 plasma. Hopefully, I will be able to adjust the
height of the resulting optic by changing the gas concentrations (with CH4
etching the glass and O2 etching the photoresist). Right now, the optics
that come out of the plasma etcher are very rough-much rougher than the
photoresist profiles that shaped them. Under a microscope, I see many cracks
in the surface of the quartz. The "bumpiness" is on the order of 1/3 of a
micron (where the optic height is 1 - 2 microns). I am running at a pressure
of 150 mTorr, with gas flow rates of 100 cc/m for CH4 and 50 cc/m for O2,
and 83 W of RF power. If anyone has experience etching glass with reflowed
photoresist, their advice would be much appreciated!



Thanks!



Patrick Lu

Stanford University

Department of Electrical Engineering

http://www.stanford.edu/~patlu

_______________________________________________
[email protected] mailing list: to unsubscribe or change your list
options, visit http://mail.mems-exchange.org/mailman/listinfo/mems-talk
Hosted by the MEMS Exchange, providers of MEMS processing services.
Visit us at http://www.memsnet.org/



reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
Tanner EDA by Mentor Graphics
MEMS Technology Review
Process Variations in Microsystems Manufacturing
Mentor Graphics Corporation