MEMSnet Home: MEMS-Talk: Ti RIE
Ti RIE
2004-04-15
Greg Chance
2004-04-21
Jason Viotty
Ti RIE
Jason Viotty
2004-04-21
Ti, can be etched in a SF6-plasma. We sometimes do this, using a
parallel-plate reactor. We use a SF6-flow of 50sccm, pressure is 50mTorr and
75W RIE-power. We achieve an etchrate of 50-60nm/min.
Good luck,

Jason

___________________________________________________________
Jason Viotty
Process Engineer
C2V
http://www.c2v.nl
___________________________________________________________



-----Original Message-----
From: Greg Chance [mailto:[email protected]]
Sent: donderdag 15 april 2004 18:13
To: [email protected]
Subject: [mems-talk] Ti RIE


Hi everyone

Would anyone be able to tell me the recipe for dry etching titanium, i.e.
what gas, pressure, plate etc? I need to etch 200 nm which has been
evaporated on a GaAs substrate.

regards
Greg Chance
Bath University Physics Dept.

_______________________________________________
[email protected] mailing list: to unsubscribe or change your list
options, visit http://mail.mems-exchange.org/mailman/listinfo/mems-talk
Hosted by the MEMS Exchange, providers of MEMS processing services.
Visit us at http://www.memsnet.org/


reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
Tanner EDA by Mentor Graphics
The Branford Group
MEMS Technology Review
Process Variations in Microsystems Manufacturing