A MEMS Clearinghouse® and information portal
for the MEMS and Nanotechnology community
RegisterSign-In
MEMSnet Home About Us What is MEMS? Beginner's Guide Discussion Groups Advertise Here
News
MEMSnet Home: MEMS-Talk: Reg: problems with SU-8 bonding to the silicon wafer
Reg: problems with SU-8 bonding to the silicon wafer
2005-06-23
Vishwanath Somashekar
2005-06-23
[email protected]
2005-06-23
Vishwanath Somashekar
Thin PDMS Films
2005-06-24
[email protected]
2005-06-25
Tolga Kaya
2005-06-27
Patrick Roman
2005-06-23
Brubaker Chad
2005-06-24
Brubaker Chad
2005-06-27
Vishwanath Somashekar
2005-06-29
Brubaker Chad
2005-06-30
Vishwanath Somashekar
Reg: problems with SU-8 bonding to the silicon wafer
Vishwanath Somashekar
2005-06-27
On 6/23/05, Brubaker Chad  wrote:
> The best suggestion I can make for the alignment is to do a simple
> masking step on the bare wafer, to put basic alignment keys (you could
> possibly even use the first level mask of the SU-8).  Then, do a shallow
> etch to define the patterns. You will then have alignment keys for the
> second layer.
>

HI,
I tried your suggestion which required that I spin the second layer
before developing the result. I have not yet tried to cast PDMS to
this microchannel and hence not sure if the layer will stick to the
wafer. However, I did notice that i see some patches on the
microchannel, which have the color of smoke. My first thought was that
I have not developed SU-8 enough. But I found that no matter how long
I develop, these pathches exist on the channel and the rest of the
wafer is absolutely free of SU-8. Have you encountered such problems
and if so what is the remedy.

Again, thanks a bunch for the help

Vishwa
reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
Nano-Master, Inc.
Mentor Graphics Corporation
Tanner EDA by Mentor Graphics
Harrick Plasma, Inc.