A MEMS Clearinghouse® and information portal
for the MEMS and Nanotechnology community
RegisterSign-In
MEMSnet Home About Us What is MEMS? Beginner's Guide Discussion Groups Advertise Here
News
MEMSnet Home: MEMS-Talk: how to process hydrophilic bonding?
how to process hydrophilic bonding?
2005-07-05
NL
2005-07-06
Sumant Sood
2005-07-07
Brubaker Chad
2005-07-08
Simon Garcia
how to process hydrophilic bonding?
Brubaker Chad
2005-07-07
In fact, if anything, the HF bearing clean would be detrimental to a
hydrophilic bond process, since that clean would remove the hydrophilic
oxide surface (to which the -OH species are attached after the RCA1
clean, which will, in turn, promote the hydrophilic bond via hydrogen
bonding).

Best Regards,
Chad Brubaker

-----Original Message-----
From:  Sumant Sood
Subject: RE: [mems-talk] how to process hydrophilic bonding?

Hi Nielei,
If your Si wafers have no particle problems (assuming they are prime
grade),
hydrophilic bonding should not be a problem. Do a RCA, SC1 Clean (5:1:1,
H2O, NH4OH, H2O2, preferably with ultrasonic or megasonics) for 15 to 20
minutes, followed by a DI rinse to activate the wafer surface.

I don't see any reason why you are you using the HNA etch
(65%HNO3:48%HF:H2O=5:100:0.001) as you mentioned prior to bonding. You
do not need this.
reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
MEMStaff Inc.
Process Variations in Microsystems Manufacturing
Harrick Plasma, Inc.
University Wafer