MEMSnet Home: MEMS-Talk: Lift- off Ti/Pt
Lift- off Ti/Pt
2009-08-20
Shah, Forum N
2009-08-20
Ruiz, Marcos Daniel (SENCOE)
2009-08-21
Huihang Dong
2009-08-21
DongJuan Xi
2009-08-21
Xiaoguang Liu
2009-08-21
Huihang Dong
2009-08-21
Brad Cantos
2009-08-22
Xiaoguang Liu
2009-08-22
Wilson, Thomas
2009-08-22
Brad Cantos
2009-08-21
mikas remeika
2009-08-22
Wilson, Thomas
2009-08-22
Brad Cantos
Lift- off Ti/Pt
Wilson, Thomas
2009-08-22
Here's one foolproof recipe for patterning sputtered metallization layers (on
silicon) as thick as 500-nm using image reversal with AZ5214E (no YES oven used)
and requires no dry etching.

Acetone+Methanol spin rinses followed by drying spin (you may also wish to do a
piranha clean first if stored in plastic chip cases for more than a month)

Dispense AZ
Spin at 4000 rpm 45 sec (1.4 micron)
Use razor blade to skim off excess PR near chip edges (if other than wafers) -
this prevents chip sticking to photomask during soft contact exposure!
Pre-bake 100 C 60 sec
Expose 320 nm @ 50 mJ (using MA-6 in soft contact mode => 3 micron lines are
easy).
Post-bake 117 +/- 2 C @60 sec
Flood Expose: 1 Joule at 365 nm AOI
Sputter up to 500 nm thick metal (I haven't pushed it to higher thicknesses)
Lift-off: Acetone soak 15 min, followed by 1-2 min sonication with acetone in
beaker floating in water bath of ultrasonicator

Thomas Wilson
Department of Physics
Marshall University


reply
Events
Glossary
Materials
Links
MEMS-talk
Terms of Use | Contact Us | Search
MEMS Exchange
MEMS Industry Group
Coventor
Harrick Plasma
Tanner EDA
University Wafer
The Branford Group
MEMS Technology Review
Mentor Graphics Corporation